E-PBF (electron beam powder bed fusion, also known as EBM) builds open lattice and trabecular structures in Ti6Al4V with struts down to 0.4 mm with the 70 ยตm parameters (line melt) and 0.35 mm with the 50 ยตm parameters (point melt). The design rule that matters most is simple: the powder inside the structure has to have a way out. This article covers strut and pore sizes, cell types, powder removal and the transition to a solid core.
New to the process? Start with What is E-PBF (electron beam powder bed fusion)?.
Trabecular structure or fine internal lattice?
Both are often called โlatticeโ, but they behave very differently in production.
Trabecular or porous structure: an open-cell structure on the surface of a part, for example the bone-ingrowth surface of an acetabular cup or a spinal implant. The struts are relatively coarse and the structure is open to the outside. This is where E-PBF is strong.
Fine internal lattice: a fine structure enclosed inside a part, with no open path to the surface. In E-PBF the powder inside sinters during the build and cannot be removed from a fully enclosed volume.
The rest of this article is about open lattice and trabecular structures.
Hip cup with an open trabecular surface, built with E-PBF.
Design ranges
All values are for Ti6Al4V on a Colibrium Additive Spectra L. Measured values come from ISO/ASTM 52902 test artifacts.
70 ยตm (line melt) | 50 ยตm (point melt) | |
|---|---|---|
Smallest lattice strut, measured | 0.4 mm | 0.35 mm |
Smallest gap or opening, measured | 0.4 mm | 0.4 mm |
The measured values are the limits of the process. A typical trabecular design for serial production sits comfortably inside them:
Typical trabecular design | Value |
|---|---|
Strut thickness | Around 0.4 mm |
Pore size | Around 600 ยตm |
Lattice depth from the open surface | Around 2 mm |
These values match what published orthopedic implant designs commonly use for bone ingrowth: pores of a few hundred micrometers and porosities in the range of 60 to 80 %. The right values for a specific implant depend on its function and are set by the OEM. AIMโs role is to make sure the design builds reliably and can be cleaned.
More on measured feature sizes in What feature sizes can E-PBF achieve in titanium?.
Rule 1: give the powder a way out
During an E-PBF build, the powder around the part is lightly sintered. That sintered powder fills every pore of a lattice. After the build, it is removed by blasting, so it has to be reachable from the outside.
An open lattice lets the sintered powder be blasted out through the surface. In a fully enclosed lattice, the powder has no way out. The cell size and depth follow a typical design: 0.4 mm struts, pores around 600 ยตm and a lattice depth of 2 mm.
Keep the cells open. Every pore should connect to its neighbors and, through them, to an outer surface.
Keep the depth in mind. The further a pore sits from an open surface, the harder it is to blast clean. With pores around 600 ยตm, a lattice depth of around 2 mm from the nearest open surface cleans reliably, which covers the trabecular layer on a typical acetabular cup. The depth counts from the nearest opening, so a porous section that is open on two sides can be thicker. Deeper or finer structures are assessed per design.
Open up larger cells toward the surface, if the design allows, so the blast media can reach deeper.
Avoid closed cavities inside the lattice or between the lattice and the solid core.
Rule 2: choose a cell type that suits the process
Strut-based unit cells, such as diamond, dodecahedron or octet cells, are well suited to E-PBF. They are open in all directions, which helps powder removal.
Stochastic or randomized structures, which mimic cancellous bone, also build well, as long as the struts stay above the minimum size and the pores stay open.
Sheet-based structures, such as gyroids, behave like thin walls rather than struts. Keep the sheet thickness above the minimum wall thickness of around 0.75 mm.
Rule 3: design the transition to the solid core
Where the lattice meets the solid body of the part, the connection carries the load. A few rules:
Let the struts grow into the solid body, instead of ending flush against it, so each strut has a proper root.
Avoid sudden jumps in thickness between the lattice and a thin solid wall.
Check the interface for closed pockets, where powder could be trapped between the lattice and the solid.
Where the limits are
E-PBF is not the right process for every lattice. Fully enclosed fine lattices, with no route out for the powder, cannot be cleaned and fall outside what the process can deliver. Very fine struts, below the sizes in the table above, are also outside the range. When a design falls into these groups, AIM will say so early.
Designing with AIM
Lattice design is one step in AIMโs work from feasibility to serial production: design review, lattice design, process development, qualification and serial production. AIM can review an existing lattice design for buildability and cleaning, or work with the customer on the design from the start.