On AIM’s Spectra L, E-PBF (electron beam powder bed fusion, also known as EBM) builds Ti6Al4V lattice struts down to 0.35 mm, solid walls down to 0.73 mm and gaps down to 0.4 mm, as built. As-built surface roughness on vertical surfaces is Ra 12 to 16 µm, and general tolerances are ±0.3 mm, or ±0.1 mm on small features. The values below were measured on ISO/ASTM 52902 test artifacts, with both the 70 µm (line melt) and 50 µm (point melt) parameters.
New to the process? Start with What is E-PBF (electron beam powder bed fusion)?.
Measured feature sizes
All values are for Ti6Al4V, as built on a Colibrium Additive Spectra L, measured on ISO/ASTM 52902 geometric test artifacts.
Feature, as built | 70 µm (line melt) | 50 µm (point melt) |
|---|---|---|
Smallest lattice strut ¹ | 0.4 mm | 0.35 mm |
Thinnest wall | 0.77 mm | 0.73 mm |
Thinnest pin | 0.75 mm | 0.72 mm |
Smallest gap or slot | 0.4 mm | 0.4 mm |
Smallest hole tested | 0.5 mm | 0.5 mm |
Surface roughness Ra, vertical surfaces ² | 12 to 13 µm | 12 to 16 µm |
¹ Built with parameters tailored for lattice structures. ² From Colibrium Additive process validation reports.
Tolerances: ±0.3 mm in general, ±0.1 mm on small features.
Line melt or point melt?
Both melt strategies resolve the same features, within a few hundredths of a millimeter. The difference lies elsewhere. Point melting fuses the powder through individual points instead of continuous lines, which gives finer control of the energy put into each area. That makes it possible to build inclined and down-facing surfaces without supports. Line melting with 70 µm layers builds faster, which lowers the cost per part when the geometry allows it.
The choice is made per part. More in What is point melt, and when can a part be built without supports? and Supports in E-PBF: a choice, not a requirement.
Why E-PBF features are larger than L-PBF features
E-PBF builds coarser features than laser powder bed fusion (L-PBF). Three things set the limit:
Beam power and melt pool size. E-PBF melts with far more power per beam. With AIM’s 70 µm parameters (line melt), the beam runs at 28 mA and 60 kV, which is about 1.7 kW. The L-PBF systems most common in implant production use lasers of around 400 W each, and even high-power lasers rarely exceed about 1 kW. More power gives a larger melt pool, which builds faster but cannot resolve as fine a detail as a small laser spot.
Powder size. E-PBF uses powder of 45 to 106 µm, against around 25 to 63 µm for L-PBF. A feature cannot be much finer than a few powder particles.
Sintered powder on the surface. The powder around the part is lightly sintered during the build, and some of it bonds to the part surface. This is the main source of the as-built roughness.
The same coarse powder and sintered powder bed are what make E-PBF cost-effective for serial production: cheaper powder, parts stacked in several levels, and no stress relief. For most implants and industrial parts the feature sizes above are more than sufficient.
Surface roughness
As-built Ra of 12 to 16 µm applies to vertical surfaces. Roughness varies with surface orientation: down-facing surfaces are typically rougher. Functional surfaces, such as tapers, threads, sealing faces and bearing seats, are machined. For porous bone-ingrowth surfaces on implants, the as-built texture is part of the design.
Holes and internal channels
Holes down to 0.5 mm were resolved in testing. For internal channels, the limit is usually not the build but the cleaning: after the build, the sintered powder inside a channel has to be blasted out. Short, straight channels with open ends are straightforward. Long, narrow or winding channels need to be reviewed case by case, and AIM will assess this early in a feasibility review.
Build envelope
System | Build envelope | Units at AIM |
|---|---|---|
Spectra L | Ø350 × 430 mm | 1 |
Q20plus | Ø350 × 380 mm | 3 |
Q10plus | 200 × 200 × 180 mm | 2 |
Since parts are held in the sintered powder cake rather than anchored to the build platform, the full build height can be used, with parts stacked in several levels.
Design guidelines in short
Keep solid walls at 0.8 mm or more for margin above the measured 0.73 to 0.77 mm.
Lattice struts can go down to 0.35 mm with the 50 µm parameters and 0.4 mm with the 70 µm parameters.
Keep gaps and slots at 0.4 mm or more.
Add around 1 mm machining allowance on functional surfaces as a general starting point.
Give internal channels open ends and a straight path for powder removal.
Apply ±0.3 mm general tolerance to as-built features, and machine where tighter tolerances are needed.
ISO/ASTM 52911-3 gives general design guidance for PBF-EB/M. For a specific part, the quickest route is a conversation: send AIM a drawing or a CAD file, and AIM will come back with a view on build strategy, critical features and cost.
When L-PBF is the better fit
L-PBF is usually the better route when a part needs walls thinner than about 0.75 mm, an as-built Ra below about 10 µm without machining, or long, narrow internal channels. If a design falls into these groups, AIM will say so early.