Point melt is a way of melting each layer in E-PBF (electron beam powder bed fusion, also known as EBM) where the electron beam fuses the powder point by point instead of in continuous lines. The energy input is spread more evenly across the layer, which gives more uniform material properties and makes it possible to build inclined and down-facing surfaces without supports. The trade-off is build time: point melt runs with thinner layers, so it suits parts where surface and geometry matter more than build speed.
New to the process? Start with What is E-PBF (electron beam powder bed fusion)?.
How point melt works: from lines to points
The hardest surfaces to build in any powder bed process are the ones facing down. Under an overhang, each new layer is melted on top of powder instead of solid metal. Powder conducts far worse than solid titanium, so the energy put in there cannot get away as quickly. Too much energy gives a rough, uneven down-facing surface. In E-PBF, that is the main reason supports are still used under some overhangs: they carry the energy away.
The answer is to control how much energy goes in, and where. Point melt takes that control a big step further.
The same layer melted two ways. Line melt traces contours and fills the inside with hatch lines. Point melt does the same with individual points: point contours along the edge and a field of points inside.
Before: energy controlled along each line
With line melt, the beam first traces a few contours around the edge of each cross-section and then fills the inside with parallel hatch lines. Energy is controlled through beam speed and power. A so-called thickness function lowers the energy where there are only a few millimeters of solid material between the layer and the powder below, so the material just above an overhang gets less energy than the bulk of the part. Readers coming from laser powder bed fusion (L-PBF) will recognize the idea from down-skin parameters.
This works, but it has a limit. The energy can be changed along a line, while the timing cannot. Each line is melted in a single pass, and every spot on it then idles until the beam comes past with the next line. How long the melt pool gets to cool down is decided by the scan pattern, line by line.
Now: energy and cooldown controlled per point
With point melt, the beam melts the whole layer as individual points, contours included: rows of points follow the edge, and the inside is filled with a field of points. The beam jumps between them instead of sweeping lines. An electron beam is steered by magnetic coils with no moving parts, so it can jump almost instantly. Every point gets two settings of its own:
Energy: the beam power and how long the beam stays on the point.
Cooldown: how long the point is left to idle before the beam melts the points next to it.
With line melt, energy varies along each line, but cooldown is set line by line by the scan pattern. With point melt, every point has its own energy and its own cooldown.
Energy control goes from per line to per point, and cooldown, which until now could only be controlled per line, can be controlled per point as well. The illustration above shows the difference.
Under an overhang, energy is reduced close to the powder so the down-facing surface does not get more energy than it can take.
Close to powder, energy and cooldown are tuned point by point, so the down-facing surface gets exactly the energy it can take. That is what makes inclined and down-facing surfaces possible without supports. The more even energy input across each layer also gives more uniform material properties.
On the Colibrium Additive Spectra L, point melt runs with 50 ยตm layers, against 70 ยตm for line melt.
What point melt changes
70 ยตm (line melt) | 50 ยตm (point melt) | |
|---|---|---|
Melt pattern | Continuous lines | Individual points |
Layer thickness | 70 ยตm | 50 ยตm |
Build speed | Faster | Slower |
Inclined and down-facing surfaces | Supports often used | Can be built without supports |
Yield strength, Grade 23, as built | 892 to 913 MPa | 933 to 938 MPa |
Elongation, Grade 23, as built | 14 to 16 % | Around 13 % |
Difference between build directions | Small | Almost none |
Thinnest wall, as built | 0.77 mm | 0.73 mm |
Smallest lattice strut | 0.4 mm | 0.35 mm |
Surface roughness Ra, vertical surfaces | 12 to 13 ยตm | 12 to 16 ยตm |
Mechanical values are averages from AIMโs machine qualification and Colibrium Additiveโs process verification. Feature sizes were measured on ISO/ASTM 52902 test artifacts. Details in What mechanical properties does E-PBF Ti6Al4V have? and What feature sizes can E-PBF achieve in titanium?.
Three differences matter most in practice:
More uniform properties. Strength is almost the same whether the part is built vertically or horizontally. AIMโs experience suggests the reason is a more uniform microstructure: melting point by point appears to break up the columnar grains that are typical of line melt.
Higher strength. In the data so far, Grade 23 yield strength is about 25 to 40 MPa higher than with line melt, at slightly lower elongation. The builds used different powder lots, so part of the difference may come from the powder. Both are well above the ASTM F3001 minimums.
Freer geometry. Inclined and down-facing surfaces can be built without supports, which opens up more build orientations.
Feature resolution, on the other hand, is almost the same. Both strategies resolve walls, pins and gaps within a few hundredths of a millimeter of each other.
When can a part be built without supports?
Acetabular augments built without supports using point melt, in trials at Colibrium Additive.
In any E-PBF build, the sintered powder cake around the part carries it and conducts the energy away. Nothing has to be anchored to the build platform, so supports are never needed to hold a part in place, as they are in laser powder bed fusion (L-PBF).
Where supports are still used in E-PBF, it is mainly under large inclined or down-facing surfaces, to carry energy away and get a good surface. With energy and cooldown controlled per point, point melt handles those surfaces without supports.
Whether a part should be built without supports is a cost and capability decision:
Without supports (point melt): no support removal, a clean as-built surface on down-facing areas, more freedom in orientation. The thinner layers mean a longer build.
With supports (line melt): a faster build with 70 ยตm layers, and a lower cost per part. Supports are removed afterwards.
Spinal implants built without supports using point melt, in trials at Colibrium Additive.
Support-free builds suit smaller parts best, where build time is not the main cost driver and the surface or geometry is. For larger parts, a few well-placed supports with line melt are often the better choice. AIM makes that call per part, together with the customer. More in Supports in E-PBF: a choice, not a requirement.
Where AIM uses point melt
AIM runs point melt in production today: on the Q20plus for titanium FreeFlowยฎ tooling for molded fiber packaging, with AIMโs own point melt parameters, and on the Spectra L for HIPed impellers. AIM has worked with point melt since 2019, in four Vinnova-funded projects. More in How long has AIM worked with point melt?. For new parts, point melt and line melt are compared early in the project, and the choice is made on cost, surface and geometry.
When point melt is not the right choice
Point melt does not change the basic limits of E-PBF. Very thin walls, very fine features and long, narrow internal channels are still better suited to L-PBF or machining. And when a part is large and the as-built surface on down-facing areas does not matter, line melt with a few supports is usually faster and cheaper.